Name:Tungsten Nickel Iron Rod
Material:W90-97NiFe(Magnetic)&W90-97NiCu(Nonmagnetic)
Density:16.8-18.8g/cm3
Property of tungsten alloy
AMST 21014 class 1
90%WNiFe, 90%WNiCu
Density : 17.0
Hardness: 32HRC max
Elongation: 5-20%
- Tungsten Nickel Copper Alloy
Tungsten Nickel Iron Rod Method
1), Blending of tungsten powder with other metal powders and a
bonding agent, cooling and sieving.
2), Pressing the blended powder to the required shape (allowing for
shrinkage during the final processing), and shaping the green part
component.
3). Pre-sintering the pressed components to remove the bonding
agent.
Final sintering in the hydrogen fed furnace to fuse the powder
particles together.
4). Supplied in bar, square, round and rectangle sizes are
available in rough oversize, or turned or ground to exact
requirements. Components can also be produced to customer drawings.
Tungsten Nickel Iron Rod Picture:
Technical datasheet for Tungsten Nickel Iron Rod
Tungsten heavy alloy | W-Ni-Fe | W-Ni-Cu | |||||
Designation | 90W | 92.5W | 95W | 97W | 90Cu | 92.5Cu | 97Cu |
Density (g/cm3) | 17.0 | 17.6 | 18.0 | 18.5 | 17.0 | 18.0 | 18.5 |
Tensile Strength (MPa) | 820 | 780 | 820 | 840 | 750 | 650 | 550 |
Elongation (%) | 10 | 7.0 | 7.0 | 5.0 | 1.2 | 1.0 | 0.5 |
Hardness (HRC) | 25 | 26 | 27 | 28 | 24 | 27 | 28 |
Young's Modulus (GPa) | 310 | 320 | 340 | 365 | 270 | 300 | 320 |
Thermal expansion coefficients (10-6/K) | 4.61 | 4.62 | 4.60 | 4.50 | 5.60 | 4.40 | 4.00 |
Electrical conductivity (%) | 10 | 13 | 13 | 17 | 17 | 19 | 23 |
Thermal conductivity (W/m.K) | 80 | 90 | 93 | 95 | 110 | 120 | 125 |